PPS
PPS
PPS(Polyphenylene Sulfide)´Â Ä¡¼ö¾ÈÁ¤¼ºÀÌ °¡Àå ¶Ù¾î³ Çöó½ºÆ½ Áß Çϳª·Î, Ź¿ùÇÑ ³»ÈÇмº ¹× ³»¿¼ºÀ» µ¿½Ã¿¡ °¡Áö°í ÀÖ¾î °í¿ÂÀÇ ³»ÈÇмºÀÌ ¿ä±¸µÇ´Â ÈÇÐÇ÷»Æ®, ÀǾàÇ°, ¹ÝµµÃ¼ Á¦ÀÛ°øÁ¤ µî Á¤¹Ð±â±âºÎÇ°À¸·Î ´Ù¾çÇÏ°Ô »ç¿ëµÇ°í ÀÖ´Ù. °¢ Makerº°·Î »óÀÌÇÑ »óÇ¥(Trade Name)·Î Á¦Ç°À» ÆǸÅÇÏ°í Àִµ¥ Ryton(Chevron Phillips Chemical), Techtron(Äâµå¶õÆ®)ÀÌ ´ëÇ¥ÀûÀÌ´Ù
Ư¡
220¡É±îÁö ¶Ù¾î³ °µµ °æµµ À¯Áö(-20¡É)
Ź¿ùÇÑ ³»ÈÇмº(200¡É ÀÌÇÏ¿¡¼ ¹ÝÀÀÇÏ´Â À¯±â¿ëÀç ¾øÀ½)
¼öºÐÈí¼öÀ² °ÅÀÇ ¾øÀ½
¶Ù¾î³ ½ºÆÀ³»¼º
³»¹æ»ç¼º
³·Àº ¿ÆØâ°è¼ö(Ä¡¼ö ¾ÈÁ¤¼º)
Ź¿ùÇÑ Àü±âÀû Ư¼º
³»È¿°¼º(UL94 V-0 ±Þ)
PHYSICAL PROPERTIES
Natural type of PPS
|
UNITS
|
ASTM
|
RESULTS
|
Density
|
lb/in3
|
D792
|
0.049
|
Water Absorption, 24 hrs
|
%
|
D570
|
0.01
|
MECHANICAL PROPERTIES
|
UNITS
|
ASTM
|
RESULTS
|
Tensile Strength
|
psi
|
D638
|
13500
|
Tensile Modulus
|
psi
|
D638
|
500000
|
Tensile Elongation @Break
|
%
|
D638
|
15
|
Flexural Strength
|
psi
|
D790
|
21000
|
Flexural Modulus
|
psi
|
400000
|
575000
|
Compressive Strength
|
psi
|
D695
|
21500
|
Compressive Modulus
|
psi
|
D695
|
430000
|
Hardness, Rockwell R
|
|
D785
|
R125/M95
|
IZOD Impact Strength Notched
|
ft-lb/in
|
D256
|
0.6
|
THERMAL PROPERTIES
|
UNITS
|
ASTM
|
RESULTS
|
Coefficient of Linear Thermal Expansion
|
(x 10-5 in./in./¡ÆF)
|
D256
|
2.8
|
Heat Deflection Temp at 264 psi
|
¡ÆF
|
|
250
|
Max Operating Temp
|
¡ÆF
|
|
425
|
Thermal Conductivity
|
BTU-in/ft2-hr-¡ÆF
|
C177
|
2
|
Flammability Rating
|
|
UL94
|
V - O
|
ELECTRICAL PROPERTIES
|
UNITS
|
ASTM
|
RESULTS
|
Dielectric Strength
|
V/mil
|
D149
|
540 @1/8" th.
|
Dielectric Constant @ 1 MHz
|
|
D150
|
3
|
Dissipation Factor @ 1 MHz
|
|
D150
|
0.0013
|
Volume Resistivity, 50% RH
|
ohm-cm
|
D257
|
4.5 x 101
|
TYPICAL PROPERTIES of EXTRUDED TECHTRON PPS &PEEK GRADES
|
ASTM or UL test
|
Property
|
Techtron PPS Unfilled
|
Techtron HPV Bearing Grade
|
PEEK Unfilled
|
Ketron HPV Bearing Grade
|
PHYSICAL
|
D792
|
Density (lb/in©ø) (g/cm©ø)
|
0.049 1.35
|
0.052 1.43
|
0.047 1.31
|
0.052 1.44
|
D570
|
Water Absorption, 24 hrs (%)
|
0.01
|
0.01
|
0.01
|
0.005
|
D570
|
Water Absorption, Saturation (%)
|
0.03
|
0.09
|
0.05
|
0.03
|
MECHANICAL
|
D638
|
Tensile Strength (psi)
|
13,500
|
10,900
|
16,000
|
11,000
|
D638
|
Tensile Modulus (psi)
|
500,000
|
540,000
|
500,000
|
850,000
|
D638
|
Tensile Elongation at Break (%)
|
15
|
5
|
20
|
2
|
D790
|
Flexural Strength (psi)
|
21,000
|
10,500
|
25,000
|
27,500
|
D790
|
Flexural Modulus (psi)
|
575,000
|
535,000
|
600,000
|
1,100,000
|
D695
|
Compressive Strength (psi)
|
21,500
|
15,500
|
20,000
|
26,700
|
D695
|
Compressive Modulus (psi)
|
430,000
|
340,000
|
500,000
|
1,000,000
|
D785
|
Hardness, Rockwell
|
M95/R125
|
M84
|
M100/R126
|
M85
|
D256
|
IZOD Impact Notched (ft-lb/in)
|
0.6
|
1.4
|
1.0
|
0.7
|
PTM55007 (not ASTM)
|
Coefficient of Friction, Dynamic
|
0.4
|
0.2
|
0.4
|
0.21
|
PTM55007 (not ASTM)
|
Limiting PV (psi-fpm)
|
3,000
|
8,750
|
8,500
|
35,000
|
PTM55007 (not ASTM)
|
"k" wear factor, (x 10-10 in3-min/lb-ft-hr)
|
2,400
|
62
|
375
|
100
|
THERMAL
|
D696
|
Coefficient of Linear Thermal Expansion (x 10-5 in./in./¡ÆF)
|
2.8
|
3.3
|
2.6
|
1.7
|
D648
|
Heat Deflection Temp (¡ÆF / ¡ÆC) at 264 psi
|
250 / 121
|
240 / 115
|
320 / 160
|
383 / 195
|
D3418
|
Melting Temp (¡ÆF / ¡ÆC)
|
540 / 282
|
536 / 280
|
644 / 340
|
644 / 340
|
-
|
Max Operating Temp (¡ÆF / ¡ÆC)
|
425 / 218
|
430 / 221
|
480 / 249
|
482 / 250
|
C177
|
Thermal Conductivity (BTU-in/ft©÷-hr-¡ÆF) (x 10-4 cal/cm-sec-¡ÆC)
|
2.0 6.9
|
2.1 7.2
|
1.8 6.2
|
1.7 5.9
|
UL94
|
Flammability Rating
|
V-0
|
V-0
|
V-0
|
V-0
|
ELECTRICAL
|
D149
|
Dielectric Strength (V/mil) short time, 1/8" thick
|
540
|
500
|
480
|
-
|
D150
|
Dielectric Constant at 1 MHz
|
3.0
|
-
|
3.3
|
-
|
D150
|
Dissipation Factor at 1 MHz
|
0.0013
|
-
|
0.003
|
-
|
D257
|
Surface Resistivity (ohm-square) at 50% RH
|
1013
|
1013
|
1013
|
104
|
|